Open Access

Cellular response of chondrocytes to magnesium alloys for orthopedic applications

  • Authors:
    • Yi Liao
    • Qingli Xu
    • Jian Zhang
    • Jialing Niu
    • Guangyin Yuan
    • Yao Jiang
    • Yaohua He
    • Xinling Wang
  • View Affiliations

  • Published online on: May 14, 2015     https://doi.org/10.3892/ijmm.2015.2211
  • Pages: 73-82
  • Copyright: © Liao et al. This is an open access article distributed under the terms of Creative Commons Attribution License [CC BY_NC 3.0].

Metrics: Total Views: 0 (Spandidos Publications: | PMC Statistics: )
Total PDF Downloads: 0 (Spandidos Publications: | PMC Statistics: )


Abstract

In the present study, the effects of Mg-Nd-Zn-Zr (JDBM), brushite (CaHPO4·2H2O)-coated JDBM (C-JDBM), AZ31, WE43, pure magnesium (Mg) and Ti alloy (TC4) on rabbit chondrocytes were investigated in vitro. Adhesion experiments revealed the satisfactory morphology of chondrocytes on the surface of all samples. An indirect cytotoxicity test using MTT assay revealed that C‑JDBM and TC4 exhibited results similar to those of the negative control, better than those obtained with JDBM, AZ31, WE43 and pure Mg (p<0.05). There were no statistically significant differences observed between the JDBM, AZ31, WE43 and pure Mg group (p>0.05). The results of indirect cell cytotoxicity and proliferation assays, as well as those of apoptosis assay, glycosaminoglycan (GAG) quantification, assessment of collagen Ⅱ (Col Ⅱ) levels and RT-qPCR revealed a similar a trend as was observed with MTT assay. These findings suggested that the JDBM alloy was highly biocompatible with chondrocytes in vitro, yielding results similar to those of AZ31, WE43 and pure Mg. Furthermore, CaHPO4·2H2O coating significantly improved the biocompatibility of this alloy.

Introduction

Magnesium (Mg) and its alloys are susceptible to dissolution in aqueous solutions due to their extremely low corrosion potential, particularly in alloys containing chloride ion electrolytes (1). For this reason, Mg alloys have attracted considerable attention as potential implant materials (28). The interest in Mg alloys has been primarily motivated by their biocompatibility, biodegradability and desirable mechanical properties. For instance, the tensile strength and elastic modulus of Mg alloys are closer to those of bone, as compared with the commonly used steel and titanium alloys (28). A previous in vivo study suggested that Mg alloy implantation in animal models promoted new bone formation and biocompatibility (2). Therefore, Mg and Mg alloys may be used as biodegradable materials for orthopedic implants.

The Mg alloys that have been investigated as implant materials are mostly commercial alloys designed for the transportation industry (8). Most of these commercial Mg alloys contain aluminium (Al) and rare earth metals. However, Al is neurotoxic (9), whereas severe hepatotoxicity has been detected following the administration of rare earth metals (10). Therefore, the exploration of novel non-toxic or low-toxicity Mg alloy systems has become a research highlight.

In this study, a medical Mg alloy, designated as Mg-Nd-Zn-Zr (JDBM), was further evaluated for its cytocompatibility in vitro. This alloy contains a Mg matrix and approximately 3% rare earth metals (11). Preliminary results revealed that JDBM possessed favorable in vitro biocompatibility to rabbit chondrocytes (12). In this study, rabbit chondrocytes were further used as an in vitro model to evaluate the effects of JDBM, brushite (CaHPO4·2H2O)-coated JDBM (C-JDBM), AZ31, WE43, pure Mg and Ti alloys (TC4). The effects of the Mg and Mg alloys on the adhesion, viability, proliferation and apoptosis of chondrocytes were investigated. The glycosaminoglycan (GAG) and collagen II (Col II) content, as well as the mRNA expression of Col II and aggrecan were also investigated.

Materials and methods

Sample and extract preparation

JDBM was previously developed for biomaterial applications by our group (11). C-JDBM, the commercial Mg alloys, WE43 and AZ31, pure Mg (Shanxi Yanbixin Magnesium Co., Ltd., Shanxi, China), and the Ti alloy, TC4 (Daiyuan, Shanghai, China), were analyzed for comparison. The detailed preparation of these materials has been described in our previous study (11).

Disk samples, 10 mm in diameter and 2.0 mm in height, were obtained by electrode discharge machining from the extruded JDBM, WE43, AZ31 and TC4 rods, as well as from high-purity Mg ingots (99.99%). All samples were ground using SiC paper of up to 1,200 grit and polished with 1 µm diamond abrasive paste, followed by a series of ultrasonic cleaning in acetone, ethanol and distilled water. The details of the CaHPO4·2H2O treatment of the JDBM disc, including the fabrication of the coating and the evaluation of its properties are described in another study of ours (13). Prior to the in vitro cytocompatibility experiments, the samples were sterilized with ethylene oxide for 24 h.

Sample extracts were prepared according to ISO 10993. The disk samples were immersed in 1.7584 ml Dulbecco’s modified Eagle’s medium with F12 (DMEM/F12) supplemented with 10% fetal bovine serum (FBS) (both from Gibco-BRL, Carlsbad, CA, USA), with a surface area-to-extraction medium volume ratio of 1.25 cm2/ml. The samples were then incubated in a humidified atmosphere with 95% humidity and 5% CO2 at 37°C for 72 h. The supernatant was collected, and the obtained extracts were refrigerated at 4°C and used within 3 days.

Chondrocyte harvest and culture

Chondrocytes were isolated from aseptically harvested articular cartilage from the knee joints of adult New Zealand rabbits weighing 2.0–2.5 kg. The cartilage samples were rinsed in sterile phosphate-buffered saline (PBS) (pH 7.4; Gibco-BRL) containing penicillin and streptomycin (100 U/ml and 100 µg/ml, respectively) (HuaBei, Shijiazhuang, China). The samples were then cut into 1–2 mm3 fragments, placed in a spinner flask containing 0.25% trypsin-EDTA (Gibco-BRL) at 37°C for 30 min, and rinsed thrice in sterile PBS. The slices as prepared samples were subsequently digested with 0.2% Col II (Sigma, St. Louis, MO, USA) in sterile PBS at 37°C for a further 12–16 h. The chondrocytes were then harvested, counted and seeded onto 25 cm2 culture flasks at a cell density of 2×104/cm2 in DMEM/F12 with 10% FBS (Gibco-BRL). The cells were then cultured in an incubator (Thermo 8000; Thermo Fisher Scientific, Inc., Shanghai, China) at 37°C with 95% humidity and 5% CO2 for 7–10 days. The cell culture medium was replenished every 3 days. The cells were passaged when they reached 80–90% confluence. Cells at passage 2 were used for further experiments.

Cell adhesion assay

Cell suspensions of 1.5 ml each were seeded into 24-well plates containing the JDBM, C-JDBM, AZ31, WE43, pure Mg and TC4 disc samples, at a cell density of 1×105 cells/ml. The culture medium was replenished daily. The cultures were incubated in a humidified atmosphere (95%) with 5% CO2 at 37°C. The samples were collected after 1 and 3 days of incubation and washed thrice with PBS (pH 7.4; Gibco-BRL) to remove the non-adherent cells. The cells were then fixed in 2.5% glutaraldehyde (Boster, Wuhan, China) solution at room temperature for 2 h followed by rinsing thrice with PBS. Following gradient ethanol dehydration (50, 60, 70, 80, 90 and 100%; for 10 min gradient ethanol dehydration), the samples were dried in a hexamethyldisilazane solution (Wuhan Boster Biological Technology, Ltd.). The samples were subsequently sputter-coated with gold. The surfaces of the cell-adhered experimental samples were observed by scanning electron microscopy (SEM; FEI Quanta 250; FEI Co., Hillsboro, OR, USA). Three parallel samples were used for each experimental condition.

Another set of 6 parallel samples were treated according to the method described above. However, these samples were fixed in 4% paraformaldehyde solution (Wuhan Boster Biological Technology, Ltd.) at room temperature for 30 min and rinsed thrice with PBS (pH 7.4; Gibco-BRL), followed by staining with a 4′,6-diamidino-2-phenylindole (DAPI) solution (5 µg/ml) (Beyotime Institute of Biotechnology, Jiangsu, China) for 10 min. The samples were again rinsed thrice with PBS, for 5 min for each wash. The surfaces of the cell-adhered experimental samples were observed and recorded using an inverted phase contrast microscope (Olympus IX70; Olympus Corp., Tokyo, Japan).

Indirect cell cytotoxicity and proliferation assay

The cells cultured in DMEM/F12 alone were used as the negative controls, whereas those cultured in DMEM/F12 medium with 10% DMSO (Beyotime Institute of Biotechnology) were used as the positive controls. The cells were incubated in 96-well cell culture plates at 5×103 cells per 100 µl medium in each well for 24 h to allow attachment. The culture medium was then replaced with 100 µl of the extraction medium with the respective treatments. The 96-well cell culture plates were then observed under an optical microscope (CSW-30B; Shenzhen Coosway Optical Technology Co., Ltd, Shenzhen, China) on days 1, 3 and 5 following incubation. The culture medium was replenished every 2 days. Six parallel wells were established for each tested sample. A total of 20 µl 3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide (MTT) (Sigma) solution (5 mg/ml in PBS) was added to each well. The samples were then placed in a cell incubator for 4 h. Subsequently, 100 µl of the formazan solubilization solution [10% SDS in 0.01 MHCl (Sigma)] were added to each well and the plates were again incubated overnight in a cell incubator with a humidified atmosphere (95%) and 5% CO2 at 37°C. The spectrophotometric absorbance of the samples at 570 nm was measured using a microplate reader (Bio-Rad 680; Bio-Rad, Hercules, CA, USA).

Another set of 6 parallel 96-well cell culture plates were used to observe and record the cell morphology. The test condition was the same the as one described above, and the medium was replaced with 100 µl extraction medium. Following incubation for 1, 3 and 5 days, the 96-well cell culture plates were collected and rinsed thrice with PBS (pH 7.4; Gibco-BRL), and then stained with Alcian blue and DAPI solution (5 µg/ml) (both from Beyotime Institute of Biotechnology). The cell morphologies of the samples in the 96-well cell culture plates were observed and recorded using an inverted phase contrast microscope (Olympus IX70; Olympus Corp.). Three parallel wells were established for each stain.

Cell apoptosis assay

The chondrocytes were analyzed as follows: 7 treatment groups were set, namely, a negative control (DMEM/F12 medium), a JDBM, C-JDBM, AZ31, WE43 pure Mg and TC4 group. Cell suspensions (10 ml) were seeded into 75 cm2 culture flasks at a cell density of 1×105 cells/ml and incubated for 24 h to allow attachment. The medium was then replaced with 10 ml extraction medium or DMEM/F12 medium. The culture media were replaced after 2 days with 10 ml. Three parallel culture flasks were established for each treatment condition. Following incubation of the cells in a cell incubator for 5 days, the culture flasks were observed under an optical microscope. Chondrocyte apoptosis was assessed using the Alexa Fluor® 488 Annexin V/Dead Cell Apoptosis kit (Invitrogen Life Technologies, Carlsbad, CA, USA) with Alexa Fluor® 488 Annexin V and propidium iodide (PI) (Beyotime Institute of Biotechnology) for flow cytometry (Navios; Beckman Coulter, Inc., Brea, CA, USA). The assay was performed according to the manufacturer’s instructions.

GAG quantification assay

The quantification of the GAG content was conducted by a modification of the dimethylmethylene blue method (Beyotime Institute of Biotechnology) (14). The chondrocytes were treated as follows: the cells were seeded in 6-well cell culture plates at a density of 1×105 cells/well and incubated for 24 h to allow attachment. The medium was changed with 3 ml of extraction medium every 2 days. Following incubation of the cells under the cell culture conditions for 5 days, the 6-well cell culture plates were observed under an optical microscope. Three parallel wells were established for each treatment condition. After rinsing in PBS (pH 7.4; Gibco-BRL), a cytolysate (RIPA; Wuhan Boster Biological Technology, Ltd.) was added to each well at 0.4 ml/well and vortexed for 10 sec. An aliquot (40 µl) of the digest was assayed for the total GAG content by the addition of 200 µl of 1,9-dimethylmethylene blue dye solution (Beyotime Institute of Biotechnology). The absorbance was determined at 595 nm using a microplate reader (Bio-Rad 680; Bio-Rad). The amount of GAG was extrapolated from a standard curve based on shark chondroitin sulfate.

Col II content assay and enzyme-linked immunosorbent assay (ELISA)

The chondrocytes were treated as described above. The cells were seeded in 12-well plates at a density of 5×104 cells/well. The cells were then incubated for 24 h to allow attachment. The medium was then changed with 2 ml of extraction medium every 2 days. Following incubation of the cells in a humidified atmosphere (95%) with 5% CO2 at 37°C for 5 days, the 12-well cell culture plates were observed under an optical microscope. Three parallel wells were established for each treatment condition. After the cell culture plates were placed on ice and rinsed in PBS (pH 7.4; Gibco-BRL), a cytolysate (RIPA; Wuhan Boster Biological Technology, Ltd.) was added to each well at 0.2 ml/well, vortexed for 10 sec, and centrifuged for 10 min at 10,000 x g according to the manufacturer’s instructions. An ELISA kit (R&D Systems, Minneapolis, MN, USA) was used for the quantitative determination of rabbit Col II levels in the cell cultures from each well. ELISA was conducted according to the manufacturer’s instructions. The spectrophotometric absorbance of the samples at 450 nm was measured using a microplate reader (Bio-Rad 680; Bio-Rad). The standard curve was calculated according to the concentration and absorbance of the standard, asw ell as based on the curve to extrapolate the corresponding concentration of the sample.

RNA extraction and quantitative-reverse transcription PCR (RT-qPCR)

The chondrocytes were seeded into 25 cm2 culture flasks at a density of 4×105 cells per flask and incubated for 24 h to allow attachment. The medium was then changed with 5 ml of the respective extracts every 2 days. DMEM/F12 medium was used as a negative control. Following incubation of the cells in a humidified atmosphere (95%) with 5% CO2 at 37°C for 5 days, the culture flasks were observed under an optical microscope. Three parallel wells were established for each treatment condition. Total RNA from the chondrocytes in the different groups was isolated using TRIzol reagent (Invitrogen Life Technologies). First-strand cDNA was synthesized using the RevertAid First Strand cDNA Synthesis kit (Thermo Fisher Scientific, Inc., Waltham, MA, USA), as previously described (12). Quantitative PCR (qPCR) was performed to amplify rabbit GAPDH, aggrecan and Col II using the LightCycler DNA Master SYBR-Green I kit (Roche, Basel, Switzerland) according to the manufacturer’s instructions. The copies of target cDNA were normalized to GAPDH expression (housekeeping gene). Each PCR reaction was repeated thrice for each independent sample. The primers used were the same as those in a previous study of ours (12).

Statistical analysis

Three replicates were conducted for each test (cytotoxicity test, N=6) and are presented as the mean values ± standard deviation (SD). ANOVA for repeated measurements was used for the MTT assay data. Multivariate ANOVA and the multiple-comparison post hoc test [least significant difference (LSD)] were subsequently conducted for pairwise comparisons between groups at each time point. One-way ANOVA, followed by the multiple-comparison post hoc test [Student-Newman-Keul (SNK) test; Tukey’s test], was performed using SPSS (version 16.0) software for other group comparisons. Mauchly’s test of sphericity was used to determine whether there were any associations among the repeatedly measured data. If any (p≤0.05), multivariate ANOVA was then performed, or the Greenhouse-Geisser corrected results were taken into consideration. The effects of treatment were evaluated by estimating between subject variance. The repeated measurement effect or its interactive effect with the treatment group was evaluated by estimating within subject variance. The method of Bonferroni was used to perform pairwise comparisons of the repeatedly measured data at different measurement times in each treatment group. A value of p<0.05 was considered to indicate a statistically significant difference.

Results

Cell adhesion and morphology

The morphologies of the chondrocytes cultured on the discs of JDBM, C-JDBM, AZ31, WE43, pure Mg and TC4 for 1 or 3 days are illustrated in Figs. 1 and 2.

The chondrocytes cultured on the discs presented with a highly elongated, irregular and round shape. A few cells were already observed on the samples after 1 day of culture (Fig. 2G–I). After 3 days of culture, the number of cells on the discs increased (Fig. 2A–F). Among the cultures, a significantly greater number of adhered cells was observed on the surfaces of the C-JDBM and TC4 discs (Fig. 2A and F, respectively), whereas the least number of cells was observed on the WE43 disc (Fig. 2D).

Indirect cytotoxicity and proliferation assay

The absorbance of the chondrocytes cultured on the different extracts, DMEM/F12 and 10% DMSO media for 1, 3, and 5 days is shown in Fig. 3. The morphologies of the chondrocytes after 1, 3, and 5 days of incubation are presented in Fig. 4. As shown in Fig. 3, the absorbance of all groups of cells increased with time. As shown in Table I, the time effect (day) and the effects of day x group interaction were statistically significant (p<0.05), indicating that the research target changed with time. Furthermore, the role of the time factor varied within each group. Tests on the between-subject effects indicated that the grouping factor influenced the results, and each group of targets generally differed (p<0.05). Likewise, the absorbance of C-JDBM (Fig. 3) was greater than that of the negative control and TC4, although the difference was not significant (p>0.05). The absorbance of the remaining groups showed significantly lower results (p<0.05). By contrast, no significant differences were observed among the JDBM, AZ31, WE43 and pure Mg groups (p>0.05), thereby indicating that these alloys have high cytocompatibility with chondrocytes.

Table I

Statistical analysis of time, group factor effect and day x group interaction effect.

Table I

Statistical analysis of time, group factor effect and day x group interaction effect.

Mauchly’s test of sphericitya

Within subjects effectMauchly’s WApprox. Chi-squareDfSig.εb
Greenhouse-GeisserHuynh-FeldtLower-bound

Day0.9173.38020.1850.9231.0000.500
Tests of within subjects effects

SourceType III sum of squaresDfMean squareF-valueSig.

Day
 Sphericity assumption1.59720.798475.7910.000
 Greenhouse-Geisser1.5971.8470.865475.7910.000
 Huynh-Feldt1.5972.0000.798475.7910.000
 Lower-bound1.5971.0001.597475.7910.000
Day x group
 Sphericity assumption0.802140.05734.1320.000
 Greenhouse-Geisser0.80212.9270.06234.1320.000
 Huynh-Feldt0.80214.0000.05734.1320.000
 Lower-bound0.8027.0000.11534.1320.000
Error (day)
 Sphericity assumption0.134800.002
 Greenhouse-Geisser0.13473.8680.002
 Huynh-Feldt0.13480.0000.002
 Lower-bound0.13440.0000.003

Tests of between subjects effects

SourceType III sum of squaresDfMean squareF-valueSig.

Intercept15.060115.0603.608E30.000
Group4.43770.634151.8280.000
Error0.167400.004

{ label (or @symbol) needed for fn[@id='tfn1-ijmm-36-01-0073'] } Mauchly’s W, value of Mauchly’s W statistic; Approx. Chi-square, approximate Chi-square statistical value; Df, degrees of freedom of the Chi-square statistic; Sig., significance.

a Use of ‘Mauchly’s test of sphericity’;

b As the value was P>0.185, it need to be corrected, and we used ‘Mauchly’s W, and thus we did not need to correct the ε value ‘Greenhouse Geisser, Huynh Feldt, Lower bound’.

The analysis of cell morphology (Fig. 4) presented similar results as those of the MTT assay. A greater number of cells was observed in the negative control group (Fig. 4B), C-JDBM (Fig. 4F) and TC4 (Fig. 4H) groups after 3 days, as compared with the other groups (Fig. 4I–L), due to the loss of cells in the center of the other culture plates, while no other differences were observed between them. As shown in Fig. 4A–C and E–G, the number of cells was directly associated with the incubation time. The chondrocytes in the positive control group were extremely scarce (Fig. 4D and P), and unlike the elongated, polygonal, deltoid or irregular shape of the other chondrocytes (Fig. 4M–O and Q–T), their morphology had changed to a small and round shape (Fig. 4P), whereas the cells from all the other treatment groups appeared normal.

Apoptosis assay

The results from cell apoptosis assay (Fig. 5) were similar to those obtained by MTT assay and the analysis of cell morphology (Figs. 3 and 4). The cells cultured on C-JDBM and TC4 were comparable with those of the negative control group (p>0.05), in terms of the apoptotic rate, whereas the apoptotic rate of the cells in the other groups was higher (p<0.05). There were no statistically significant differences observed among the JDBM, AZ31, WE43 and pure Mg groups (p> 0. 05).

Total GAG quantification assay

The results obtained from the analysis of the GAG content (Fig. 6) were comparable to those obtained by MTT assay and the analysis of cell morphology (Figs. 3 and 4) and apoptosis assay (Fig. 5). The GAG content in the cells cultured on C-JDBM and TC4 was comparable to that of the negative control, while the GAG content did not differ between the cells in the other groups. There was no statistically significant difference observed in the GAG content between the JDBM, AZ31, WE43 and pure Mg groups (p>0.05).

Col II content and ELISA

The results from ELISA were not satisfactory as the values obtained for the JDBM, AZ31, WE43 and Mg samples were extremely low, much lower than those of the kit (0.1–30 ng/ml). Moreover, the negative control, as well as the C-JDBM and TC4 groups, only had values of 0.112±0.0083, 0.122±0.0068 and 0.101±0.0089 ng/ml, respectively (data not shown, as these results were lower than the lower limit of the measuring range of the kit).

RT-qPCR

As shown in Fig. 7, the results of the analysis of the relative mRNA expression levels of aggrecan and Col II in the chondrocytes following 5 days of incubation under the different treatment conditions were consistent with those obtained form the other assays (Figs. 3Figure 4Figure 56) and with the results of our previous study (12). The results revealed that the cytocompatibility of JDBM was comparable to that of AZ31, WE43 and pure Mg. Furthermore, the CaHPO4·2H2O coating significantly improved its compatibility.

Discussion

Despite numerous studies on Mg alloys for biomedical applications, the majority of these studies focused on the commercial Mg alloys that may be harmful to the human body (810). The JDBM alloy was originally developed as a Mg alloy for medical implants (11,12,15). The main aim of this study was to evaluate the cytocompatibility of JDBM to chondrocytes, which may be used for cartilage tissue engineering. The biocompatibility of different cell lines with the same Mg alloy may be significantly different (16). However, chondrocytes, widely used as ‘seed’ cells in cartilage tissue engineering, have been rarely used to study the biocompatibility of Mg alloys. Our preliminary study presented positive results (12); thus, further investigation was performed. In the present study, JDBM and C-JDBM served as the test groups, whereas the AZ31, WE43, pure Mg and TC4 alloy group were set up as the control group, aside from the negative and positive controls. Comparisons among groups revealed that JDBM and C-JDBM had better reference values as regards their cytocompatibility, based on previous positive results obtained for AZ31, WE43, and TC4 alloys, as well as pure Mg (1,2,1719).

Cell direct adhesion experiments revealed efficient chondrocyte growth, distribution and adhesion to all material surfaces (Figs. 1 and 2). The adhesion behavior of the chondrocytes is similar to that of MG-63 cells, L929 cells, human bone marrow stromal cells (hBMSCs) and MC3T3-E1 cells on the surface of Mg alloys (7,17,20,21). Furthermore, as shown in Fig. 2, the number of cells that had adhered to the surface of the C-JDBM and TC4 discs (Figs. 2A and F) was greater than that of the other groups (Fig. 2B–E), thereby indicating the better biocompatibility of chondrocytes with C-JDBM and TC4 than the others. Although the cells cultured on the WE43 alloy appeared to be fewer (Fig. 2D), the biocompatibility of WE43 is not necessarily worse than that of other non-coating materials. According to the study by Witte et al (22), the direct cell assay reduces cell viability more rapidly than the indirect cytotoxicity tests. Cells are known to be very sensitive to environmental fluctuations, including ion release, changes in pH and hydrogen evolution. The disintegrated particles and corrosion product Mg(OH)2 for Mg-based biomaterials, as well as the influencing factors increased when the cells were directly exposed to the material. To be specific, the significant increase in the pH of cell culture media caused by Mg alloy degradation may have an adverse effect on the cells (8,18,22-24). Besides, a corrosion product layer is formed during the corrosion process of Mg and Mg alloys. During immersion, the corrosion product gradually falls from the surface due to the severe mismatch between the substrate and the corrosion product layer (1). The formed corrosion product and departure process make it difficult for the cells to attach to the surface. Furthermore, the high hydrogen evolution rate affects cell attachment and proliferation. Once a Mg-based material is immersed in the cell culture medium, the hydrogen gas evolves from the sample surface, which may deteriorate cell adhesion and the ensuing proliferation process. With a high pH value, Mg(OH)2 and zinc hydroxide [Zn(OH)2] precipitate easily during the incubation period from the surface of the sample, but also in the culture medium. However, the toxicity of micro-sized Zn(OH)2 may be related to the particle concentration. Nair et al (25) indicated that micro-ZnO is extremely toxic to MG63 cells at a concentration above 100 µm (with an ~50% loss in cell viability). There were different environment fluctuations for each sample. Due to the aforementioned reasons, we changed the medium once a day to reduce the influence of these fluctuations on the cells.

The SEM micrograph revealed few chondrocytes on the TC4 disc. However, a few cells were fluorescently stained on the parallel sample (Fig. 2F). The lower adhesive force of chondrocytes, as compared with other cells may account for this result. Chondrocyte digestion possibly occurs more rapidly than other cells, including MC3T3-E1 cells in flask cultures; it only needs approximately 30–60 sec. Thus, the chondrocytes may have easily dropped off from the surface of the TC4 samples due to their complex treatment process prior to SEM. The shadows in Fig. 1F show the chondrocytes spreading and falling off. Moreover, Mg alloys have rougher surfaces following degradation than the Ti alloy, which then favors chondrocyte adhesion onto Mg alloys.

Based on indirect cell cytotoxicity and proliferation assay, the cytocompatibility of JDBM was comparable with that of AZ31, WE43 and pure Mg; however, it may be significantly improved by CaHPO4·2H2O coating. Cell viability increased with time, which was in accordance with the results obtained by direct and indirect adhesion assays (Figs. 2 and 4), as well as those of previous studies (7,16,17,20). The cell counts in parallel 96-well plates were consistent with those obtained by MTT assay and the anlaysis of cell morphology (Figs. 3 and 4). A greater number of cells was observed in the negative control, C-JDBM and TC4 groups. Some cells had disappeared from the center of the plates in the JDBM, AZ31, WE43 and pure Mg groups. The following reasons may account for these results: firstly, the obvious increase in the pH in the media caused by Mg alloy corrosion had an adverse effect on cell viability, as previously mentioned (7,8,17,19,23,24). Our preliminary results presented high pH values for uncoated samples (12); however, further and more detailed investigations are warranted to clarify this issue. Secondly, chondrocytes can be expanded in vitro in monolayer culture, although this multiplication may lead to dedifferentiation beginning from 3 or 4 passages. This process makes the cells become fibroblast-like as they lose their round phenotype and become spindle-shaped, while switching their collagen production from types II, IX and XI to types I, III and V (2629). Given the limitations of a low initial number of cells and their dedifferentiation, chondrocytes are multiplied in monolayer culture to increase the number of cells and are then transferred to a three-dimensional culture system to regain their phenotype (26,27,29). Thus, in the present study, we used cells that were passaged twice to eliminate such limitations. Apparently, the viability of the chondrocytes is inferior to that of other cells (26,27,29). Thirdly, the wells of 96-well plates are small, and surface tension brings more cell suspensions to the periphery, and more cells gathered together are more susceptible to survival than sparse ones.

The results obtained by MTT and apoptosis assays, as well as the from the analysis of GAG and Col II content alongside the relative mRNA expression of aggrecan and Col II were likewise similar. GAG, Col II, aggrecan and Col II mRNA expression are unique to chondrocytes (14,2629). The cells were visibly well attached to the coating and proliferated normally. These results can be explained by the corrosion protecting effect of the brushite coating, as discussed above, thereby improving the cytocompatibility. The purity of Mg alloys and surface modification may reduce the degradation rate of Mg and its alloys (7,17,19,20,22,30). Mg purity has improved as metallurgical techniques have improved. Surface modification includes alkali-heat treatment, carbonate treatment, ion plating deposition of Ti, surface plasma immersion ion implantation, micro-arc oxidation, fluoride coating and phosphate coating. Calcium phosphate (Ca-P) coatings are widely used on bone implant materials due to their favorable biocompatibility and osteoconductive properties (7,31). The brushite (CaHPO4·2H2O) coating has been reported to significantly improve the biocorrosion resistance and osseous integration of Mg alloys (7). In this study, CaHPO4·2H2O was coated onto JDBM alloys through chemical deposition. Compared with other surface treatment methods, the CaHPO4·2H2O coating is simpler and easier to control. Furthermore, CaHPO4·2H2O is applicable to implants of complex shapes and low-temperature processes. This last feature is of particular importance during the surface modification of Mg implants due to the low melting point of Mg (17,30). The Ca-P coating can effectively reduce the degradation rate of Mg and its alloys. Our findings confirm the excellent biocompatibility and desirable protective effects of the coated sample, which is in agreement with the results previously reported (7,17,20,30,31).

The property difference of our proposed coated and uncoated alloys may be attributed to the following reasons: firstly, the alkalization effect caused by the rapid corrosion of Mg alloys is undesirable for cell adhesion, growth and proliferation; this alkalization effect rapidly increases the pH of the SBF until pH >9.0 within approximately 2 h, which is beyond the pH range suitable for cell survival, before it finally reaches a relatively stable value of 10.5 (32). According to previously reported results, the Ca-P coating can serve as an effective corrosion inhabiting layer and reduce the increase in pH of simulated body fluid (33). Although cells are very sensitive to environmental fluctuations, particularly fluctuations in pH (2224), a Ca-P coating can improve the corrosion resistance of JDBM alloys and provide an environment for cells with a suitable pH (12,30). Thus, the Ca-P coating would likewise benefit cell adhesion and growth. The in vitro cell assays, including cell adhesion, MTT, apoptosis, GAG content assay and RT-PCR, demonstrated that C-JDBM had an excellent cellular response due to the CaHPO4·2H2O coating.

Mg and Ca ions have been previouly demonstrated to promote cell viability and proliferation, which are known to promote cell differentiation (7,34). Mg ions at an appropriate concentration can activate bone cells by influencing the protein synthesis and ancillary processes (2,34). Furthermore, Mg ion concentrations of up to 10.286 mM have been reported to be safe to human bone marrow-derived stromal cells (24). Another study demonstrated that physiologically high extracellular Mg concentrations (10 mM) enhance chondrocyte proliferation and redifferentiation in distinct concentration ranges (16). Mg is likewise known to be active in cell adhesion mechanisms (35). Furthermore, Mg hydroxide may enhance osteoblast activity and decrease the osteoclast number temporarily in peri-implant bone remodeling (36). Overall, the Mg ion and Mg(OH)2 may enhance the viability, proliferation, and adhesion ability of chondrocytes.

Finally, calcium (Ca) ions are essential in chemical signaling for cells (37). Ca ions on the material surfaces favor protein absorption, e.g., fibronectin and vitronectin, which are important cell attachment-promoting proteins. Therefore, Ca ions improve cell attachment and spreading onto the surface (38). The enhanced Mg ion concentration elevates the calcium concentration (39), which is suitable for the nucleation of the Ca-P containing compounds. This mechanism verifies that Mg is capable of osteoconductivity (39,40). Bone growth on an implant surface requires the presence of sufficient amounts of Ca and phosphate ions (17). Therefore, CaHPO4·2H2O enhances the cellular response.

The combined results show that the presence of Ca and Mg ions, together with a more stable pH, may increase cell proliferation with C-JDBM, as compared with the uncoated JDBM, AZ31, WE43 and Ti alloys or pure Mg (12).

In conclusion, in this study, the Mg alloy, JDBM, was investigated as a medical biodegradable material in terms of its cytocompatibility to chondrocytes in vitro. JDBM demonstrated high biocompatibility to chondrocytes, which was similar to the performance of AZ31, WE43 and pure Mg. The CaHPO4·2H2O coating may significantly improve its biocompatibility, which was attributed to the presence of Mg and Ca ions, as well as its more stable pH.

Acknowledgments

The present study was sponsored by grants from the Science and Technology Commission of Shanghai Municipality (11DJ1400300), the National Natural Science Foundation of China (nos. 81271961 and 51174136), and the National Key Technology Research and Development Program of China (2012BAI18B01).

References

1 

Song G, Atrens A, St John D, Wu X and Nairn J: The anodic dissolution of magnesium in chloride and sulphate solutions. Corros Sci. 39:1981–2004. 1997. View Article : Google Scholar

2 

Witte F, Kaese V, Haferkamp H, Switzer E, Meyer-Lindenberg A, Wirth CJ and Windhagen H: In vivo corrosion of four magnesium alloys and the associated bone response. Biomaterials. 26:3557–3563. 2005. View Article : Google Scholar

3 

Witte F, Fischer J, Nellesen J, Crostack HA, Kaese V, Pisch A, Beckmann F and Windhagen H: In vitro and in vivo corrosion measurements of magnesium alloys. Biomaterials. 27:1013–1018. 2006. View Article : Google Scholar

4 

Xu L, Yu G, Zhang E, Pan F and Yang K: In vivo corrosion behavior of Mg-Mn-Zn alloy for bone implant application. J Biomed Mater Res A. 83:703–711. 2007. View Article : Google Scholar : PubMed/NCBI

5 

Kannan MB and Raman RKS: In vitro degradation and mechanical integrity of calcium-containing magnesium alloys in modified-simulated body fluid. Biomaterials. 29:2306–2314. 2008. View Article : Google Scholar : PubMed/NCBI

6 

Staiger MP, Pietak AM, Huadmai J and Dias G: Magnesium and its alloys as orthopedic biomaterials: A review. Biomaterials. 27:1728–1734. 2006. View Article : Google Scholar

7 

Xu L, Pan F, Yu G, Yang L, Zhang E and Yang K: In vitro and in vivo evaluation of the surface bioactivity of a calcium phosphate coated magnesium alloy. Biomaterials. 30:1512–1523. 2009. View Article : Google Scholar

8 

Witte F, Hort N, Vogt C, Cohen S, Kainer KU, Willumeit R and Feyerabend F: Degradable biomaterials based on magnesium corrosion. Curr Opin Solid State Mater Sci. 12:63–72. 2008. View Article : Google Scholar

9 

El-Rahman SS: Neuropathology of aluminum toxicity in rats (glutamate and GABA impairment). Pharmacol Res. 47:189–194. 2003. View Article : Google Scholar : PubMed/NCBI

10 

Hirano S and Suzuki KT: Exposure, metabolism, and toxicity of rare earths and related compounds. Environ Health Perspect. 104(Suppl 1): S85–S95. 1996. View Article : Google Scholar

11 

Yuan G, Zhang X, Niu J, Tao H, Chen D, He Y, Jiang Y and Ding W: Research progress of new type of degradable biomedical magnesium alloys JDBM. Chin J Nonferrous Met. 21:2476–2488. 2011.

12 

Liao Y, Ouyang Y, Niu J, Zhang J, Wang Y, Zhu Z, Yuan G, He Y and Jiang Y: In vitro response of chondrocytes to a biodegradable Mg-Nd-Zn-Zr alloy. Mater Lett. 83:206–208. 2012. View Article : Google Scholar

13 

Niu J, Yuan G, Liao Y, Mao L, Zhang J, Wang Y, Huang F, Jiang Y, He Y and Ding W: Enhanced biocorrosion resistance and biocompatibility of degradable Mg-Nd-Zn-Zr alloy by brushite coating. Mater Sci Eng C Mater Biol Appl. 33:4833–4841. 2013. View Article : Google Scholar : PubMed/NCBI

14 

Lin YJ, Yen CN, Hu YC, Wu YC, Liao CJ and Chu IM: Chondrocytes culture in three-dimensional porous alginate scaffolds enhanced cell proliferation, matrix synthesis and gene expression. J Biomed Mater Res A. 88:23–33. 2009. View Article : Google Scholar

15 

Zhang XB, Yuan GY, Mao L, Niu JL and Ding WJ: Biocorrosion properties of as-extruded Mg-Nd-Zn-Zr alloy compared with commercial AZ31 and WE43 alloys. Mater Lett. 66:209–211. 2012. View Article : Google Scholar

16 

Feyerabend F, Fischer J, Holtz J, Witte F, Willumeit R, Drücker H, Vogt C and Hort N: Evaluation of short-term effects of rare earth and other elements used in magnesium alloys on primary cells and cell lines. Acta Biomater. 6:1834–1842. 2010. View Article : Google Scholar

17 

Geng F, Tan LL, Jin XX, Yang JY and Yang K: The preparation, cytocompatibility, and in vitro biodegradation study of pure β-TCP on magnesium. J Mater Sci Mater Med. 20:1149–1157. 2009. View Article : Google Scholar : PubMed/NCBI

18 

Popat KC, Leoni L, Grimes CA and Desai TA: Influence of engineered titania nanotubular surfaces on bone cells. Biomaterials. 28:3188–3197. 2007. View Article : Google Scholar : PubMed/NCBI

19 

Keim S, Brunner JG, Fabry B and Virtanen S: Control of magnesium corrosion and biocompatibility with biomimetic coatings. J Biomed Mater Res B Appl Biomater. 96:84–90. 2011. View Article : Google Scholar

20 

Li J, Song Y, Zhang S, Zhao C, Zhang F, Zhang X, Cao L, Fan Q and Tang T: In vitro responses of human bone marrow stromal cells to a fluoridated hydroxyapatite coated biodegradable Mg-Zn alloy. Biomaterials. 31:5782–5788. 2010. View Article : Google Scholar : PubMed/NCBI

21 

Zhang SX, Li JA, Song Y, Zhao C, Zhang X, Xie C, Zhang Y, Tao H, He Y, Jiang Y and Bian YJ: In vitro degradation, hemolysis and MC3T3-E1 cell adhesion of biodegradable Mg-Zn alloy. Mater Sci Eng C Mater Biol Appl. 29:1907–1912. 2009. View Article : Google Scholar

22 

Witte F, Feyerabend F, Maier P, Fischer J, Störmer M, Blawert C, Dietzel W and Hort N: Biodegradable magnesium-hydroxy-apatite metal matrix composites. Biomaterials. 28:2163–2174. 2007. View Article : Google Scholar : PubMed/NCBI

23 

Serre CM, Papillard M, Chavassieux P, Voegel JC and Boivin G: Influence of magnesium substitution on a collagen-apatite biomaterial on the production of a calcifying matrix by human osteoblasts. J Biomed Mater Res. 42:626–633. 1998. View Article : Google Scholar : PubMed/NCBI

24 

Yang C, Yuan G, Zhang J, Tang Z, Zhang X and Dai K: Effects of magnesium alloys extracts on adult human bone marrow-derived stromal cell viability and osteogenic differentiation. Biomed Mater. 5:0450052010. View Article : Google Scholar : PubMed/NCBI

25 

Nair S, Sasidharan A, Divya Rani VV, Menon D, Nair S, Manzoor K and Raina S: Role of size scale of ZnO nanoparticles and microparticles on toxicity toward bacteria and osteoblast cancer cells. J Mater Sci Mater Med. 20(Suppl 1): S235–S241. 2009. View Article : Google Scholar

26 

Chaipinyo K, Oakes BW and van Damme MPI: Effects of growth factors on cell proliferation and matrix synthesis of low-density, primary bovine chondrocytes cultured in collagen I gels. J Orthop Res. 20:1070–1078. 2002. View Article : Google Scholar : PubMed/NCBI

27 

Brodkin KR, García AJ and Levenston ME: Chondrocyte phenotypes on different extracellular matrix monolayers. Biomaterials. 25:5929–5938. 2004. View Article : Google Scholar : PubMed/NCBI

28 

Martin I, Suetterlin R, Baschong W, Heberer M, Vunjak-Novakovic G and Freed LE: Enhanced cartilage tissue engineering by sequential exposure of chondrocytes to FGF-2 during 2D expansion and BMP-2 during 3D cultivation. J Cell Biochem. 83:121–128. 2001. View Article : Google Scholar : PubMed/NCBI

29 

Gagne TA, Chappell-Afonso K, Johnson JL, McPherson JM, Oldham CA, Tubo RA, Vaccaro C and Vasios GW: Enhanced proliferation and differentiation of human articular chondrocytes when seeded at low cell densities in alginate in vitro. J Orthop Res. 18:882–890. 2000. View Article : Google Scholar

30 

Du H, Wei Z, Wang H, Zhang E, Zuo L and Du L: Surface microstructure and cell compatibility of calcium silicate and calcium phosphate composite coatings on Mg-Zn-Mn-Ca alloys for biomedical application. Colloids Surf B Biointerfaces. 83:96–102. 2011. View Article : Google Scholar

31 

Hench LL: Bioceramics. J Am Ceram Soc. 81:1705–1728. 1998. View Article : Google Scholar

32 

Song GL and Song SZ: A possible biodegradable magnesium implant material. Adv Eng Mater. 9:298–302. 2007. View Article : Google Scholar

33 

Xu L, Zhang E and Yang K: Phosphating treatment and corrosion properties of Mg-Mn-Zn alloy for biomedical application. J Mater Sci Mater Med. 20:859–867. 2009. View Article : Google Scholar

34 

Rude RK, Gruber HE, Wei LY, Frausto A and Mills BG: Magnesium deficiency: Effect on bone and mineral metabolism in the mouse. Calcif Tissue Int. 72:32–41. 2003. View Article : Google Scholar

35 

Paul W and Sharma CP: Nanoceramic matrices: Biomedical applications. Am J Biochem Biotechnol. 2:41–48. 2006. View Article : Google Scholar

36 

Janning C, Willbold E, Vogt C, Nellesen J, Meyer-Lindenberg A, Windhagen H, Thorey F and Witte F: Magnesium hydroxide temporarily enhancing osteoblast activity and decreasing the osteoclast number in peri-implant bone remodelling. Acta Biomater. 6:1861–1868. 2010. View Article : Google Scholar

37 

Ilich JZ and Kerstetter JE: Nutrition in bone health revisited: A story beyond calcium. J Am Coll Nutr. 19:715–737. 2000. View Article : Google Scholar

38 

Feng B, Weng J, Yang BC, Qu SX and Zhang XD: Characterization of titanium surfaces with calcium and phosphate and osteoblast adhesion. Biomaterials. 25:3421–3428. 2004. View Article : Google Scholar : PubMed/NCBI

39 

TenHuisen KS and Brown PW: Effects of magnesium on the formation of calcium-deficient hydroxyapatite from CaHPO 4·2H2O and Ca4(PO4)2O. J Biomed Mater Res. 36:306–314. 1997. View Article : Google Scholar : PubMed/NCBI

40 

Witte F, Reifenrath J, Müller PP, Crostack H-A, Nellesen J, Bach FW, Bormann D and Rudert M: Cartilage repair on magnesium scaffolds used as a subchondral bone replacement. Materialwiss Werkstofftech. 37:504–508. 2006. View Article : Google Scholar

Related Articles

Journal Cover

July-2015
Volume 36 Issue 1

Print ISSN: 1107-3756
Online ISSN:1791-244X

Sign up for eToc alerts

Recommend to Library

Copy and paste a formatted citation
x
Spandidos Publications style
Liao Y, Xu Q, Zhang J, Niu J, Yuan G, Jiang Y, He Y and Wang X: Cellular response of chondrocytes to magnesium alloys for orthopedic applications. Int J Mol Med 36: 73-82, 2015
APA
Liao, Y., Xu, Q., Zhang, J., Niu, J., Yuan, G., Jiang, Y. ... Wang, X. (2015). Cellular response of chondrocytes to magnesium alloys for orthopedic applications. International Journal of Molecular Medicine, 36, 73-82. https://doi.org/10.3892/ijmm.2015.2211
MLA
Liao, Y., Xu, Q., Zhang, J., Niu, J., Yuan, G., Jiang, Y., He, Y., Wang, X."Cellular response of chondrocytes to magnesium alloys for orthopedic applications". International Journal of Molecular Medicine 36.1 (2015): 73-82.
Chicago
Liao, Y., Xu, Q., Zhang, J., Niu, J., Yuan, G., Jiang, Y., He, Y., Wang, X."Cellular response of chondrocytes to magnesium alloys for orthopedic applications". International Journal of Molecular Medicine 36, no. 1 (2015): 73-82. https://doi.org/10.3892/ijmm.2015.2211